注: 1. 表中材料代号含义如下: C . I .――铸铁。 ASTM A48 D . I .――球墨铸造铁, ASTM A536 Steel ――铸造钢, ASTM A216 - WCA 或 WCB …… Brz.――耐酸青铜,ASTM B143A2 316SS――不锈钢,ASTM A744Gr.CF-8M AISI316 CD4Mcu ――不锈钢(双相钢), ACI CD - 4MCu Mon ――蒙乃尔 E 级, ASTMA 744Gr. M-35 Ni ――镍钢, AST MA744Gr.Cz-100 H-B ――哈氏合金 -B , ASTMA494 H-C ――哈氏合金 -C , ASTMA494 Ti ――纯钛, ASTM B367Gr. C-1 Zi ――锆 2. 表中符号含义如下 A- 满; B- 适用; C- 限制使用; × --不适用
介质 | 材料牌号 | ||||||||||
Steel C.I.D.I. | Brz | 316SS | 20合金 | CD4MCu | Mon | Ni | H-B | H-C | Ti | Zi | |
乙醛, 70 ℉ | B | A | A | A | A | A | A | A | A | A | |
醋酸, 70 ℉ | × | A | A | A | A | B | B | A | A | A | A |
醋酸, <50% ,沸点 | × | B | A | A | B | B | B | C | A | A | A |
醋酸, <50% ,沸点 | × | × | B | A | C | B | B | × | A | A | A |
丙酮,沸点 | A | A | A | A | A | A | A | A | A | A | A |
三氯化铝, <10% , 70 ℉ | × | B | C | B | C | B | C | A | B | A | |
三氯化铝, >10% , 70 ℉ | × | × | C | B | C | C | × | A | B | A | |
三氯化铝, <10% ,沸点 | × | × | × | C | × | × | × | A | × | A | |
三氯化铝, >10% ,沸点 | × | × | × | × | × | × | × | A | × | × | A |
硫酸铝, 70 ℉ | × | B | A | A | A | B | B | B | B | A | A |
硫酸铝, <10% ,沸点 | × | B | B | A | B | × | × | A | A | A | A |
硫酸铝, >10% ,沸点 | × | C | C | B | C | × | × | B | B | C | B |
氯化铵, 70 ℉ | × | × | B | B | B | B | B | A | A | A | |
氯化铵, <10% ,沸点 | × | × | B | B | C | B | B | B | A | A | A |
氯化铵, >10% ,沸点 | × | × | × | C | × | C | C | C | C | C | |
氟硅酸铵, 70 ℉ | × | × | C | B | C | × | × | C | × | × | |
硫酸铵, <40% ,沸点 | × | × | B | B | C | B | B | × | B | A | A |
砷酸 225 ℉ | × | × | C | B | C | × | × | ||||
氯化钡, <30% , 70 ℉ | × | B | C | B | C | B | B | B | B | B | B |
氯化钡, <5% ,沸点 | × | B | C | B | C | B | B | B | B | A | A |
氯化钡, >5% ,沸点 | × | C | × | C | × | C | C | C | C | C | C |
氢氧化钡, 70 ℉ | B | × | A | A | A | B | A | B | B | A | A |
硝酸钡,沸点 | C | × | B | B | B | B | B | B | B | ||
硫酸钡, 70 ℉ | C | × | B | B | B | × | × | A | A | ||
苯 ( 甲 ) 酸 | × | C | B | B | B | B | B | A | A | A | A |
硼酸,沸点 | × | C | B | B | B | C | C | A | A | B | B |
三氯化硼, 70 ℉ (干) | B | B | B | B | B | B | B | B | B | ||
三氟化硼, 70 ℉, 10%(干) | B | B | B | A | B | A | A | A | |||
盐水, 70 ℉ | × | × | × | × | × | B | B | ||||
溴 ( 干 ) , 70 ℉ | × | × | × | × | × | × | C | B | B | × | × |
溴 ( 湿 ) , 70 ℉ | × | × | × | × | × | × | C | B | × | × | |
硫酸氢钙, 70 ℉ | × | × | B | B | B | × | × | B | A | A | |
硫酸氢钙,沸点 | × | × | C | B | C | × | × | C | A | A | |
氯化钙, 70 ℉ | B | C | B | B | B | B | B | A | A | A | A |
氯化钙, <5% ,沸点 | C | C | B | B | B | A | A | A | A | A | A |
氯化钙, >5% ,沸点 | × | C | C | B | C | C | C | A | A | B | B |
氢氧化钙, 70 ℉ | B | B | B | B | B | B | B | A | A | ||
氢氧化钙, <30% ,沸点 | C | B | B | B | B | B | B | A | A | ||
氢氧化钙, >30% ,沸点 | × | × | C | C | C | C | C | B | A | ||
氯酸钙, <2% , 70 ℉ | × | × | × | C | × | × | × | A | A | A | |
氯酸钙, >2% , 70 ℉ | × | × | × | C | × | × | × | B | A | B | |
苯酚, 70 ℉ | C | B | A | A | A | A | A | A | A | A | A |
二硫化碳, 70 ℉ | B | B | A | A | A | B | B | A | |||
碳酸, 70 ℉ | B | C | A | A | A | C | B | A | A | A | A |
四氯化碳, 100% ,沸点 | B | B | A | A | A | A | A | B | B | A | A |
氯酸, 70 ℉ | × | × | × | B | C | × | × | × | C | ||
次氯酸, 70 ℉ | C | C | B | B | B | A | A | A | |||
氯乙酸, 70 ℉ | × | × | × | A | B | ||||||
氯磺酸, 70 ℉ | × | × | × | C | ` × | × | × | A | A | B | × |
铬酸, <30% | × | × | C | B | C | × | × | B | A | A | |
柠檬酸 | × | C | A | A | A | C | C | A | A | A | A |
硝酸铜, 75 ℉ | C | × | B | B | B | × | × | × | × | B | |
硫酸铜,沸点 | × | C | C | C | C | × | × | A | A | A | |
甲苯基酸 | × | C | B | B | B | C | C | B | B | ||
氯化铜 | × | C | × | × | × | C | × | C | B | × | |
氰醇, 70 ℉ | C | B | B | B | |||||||
二氯乙烷 | C | B | B | B | B | C | B | B | B | A | B |
二甘醇, 70 ℉ | A | B | A | A | A | B | B | B | B | A | A |
二硝基氯苯, 70 ℉ (干) | C | B | A | A | A | A | A | A | A | A | A |
乙醇胺, 70 ℉ | B | × | B | B | B | C | × | A | A | ||
乙醚, 70 ℉ | B | B | B | A | A | B | B | B | B | A | A |
乙醇,沸点 | A | A | A | A | A | A | A | A | A | A | A |
氯乙烷, 70 ℉ | A | B | B | B | B | B | B | B | B | A | A |
乙硫醇, 70 ℉ | C | B | B | A | B | B | B | B | B | A | A |
硫酸乙酯, 70 ℉ | C | × | B | A | B | B | B | ||||
二氯乙醇, 70 ℉ | C | B | B | A | B | B | |||||
二氯乙烯, 70 ℉ | C | B | B | B | B | B | B | B | B | A | A |
乙二醇, 70 ℉ | C | B | B | B | B | B | B | B | C | A | A |
环氧乙烷, 70 ℉ | B | B | B | B | B | B | B | A | A | A | A |
C | × | B | B | B | B | B | A | A | A | A | |
三氯化铁, <5% , 70 ℉ | × | × | × | × | × | × | × | × | A | A | B |
三氯化铁, >5% , 70 ℉ | × | × | × | × | × | × | × | × | B | B | × |
硝酸铁, 70 ℉ | × | × | B | × | B | × | × | B | |||
硫酸铁, 70 ℉ | × | × | C | B | C | C | C | B | B | B | |
硫酸亚铁, 70 ℉ | × | C | C | B | C | C | C | B | B | A | A |
甲醛,沸点 | B | B | A | A | A | B | B | B | B | A | A |
甲酸, 212 ℉ | × | C | × | A | B | C | C | A | A | C | A |
氟立昂, 70 ℉ | A | A | A | A | A | A | A | A | A | A | A |
盐酸, <1% , 70 ℉ | × | × | C | B | C | B | B | B | A | B | A |
盐酸, 1%~20% , 70 ℉ | × | × | × | × | × | × | × | B | C | × | A |
盐酸, >20% , 70 ℉ | × | × | × | × | × | × | B | C | × | B | |
盐酸, <0.5% , 175 ℉ | × | × | C | C | C | × | × | A | C | × | A |
盐酸, 0.5%~2% , 175 ℉ | × | × | × | × | × | × | B | C | × | A | |
氢氰酸, 70 ℉ | × | × | C | B | C | C | C | C | C | ||
双氧水, <30% , <150 ℉ | C | × | B | B | B | B | B | B | B | A | A |
氢氟酸, <20% , 70 ℉ | × | B | × | B | C | C | C | C | B | × | × |
氢氟酸, >20% , 50 ℉ | × | C | × | C | × | C | C | C | B | × | × |
氢氟酸,沸点 | × | × | × | × | × | C | × | C | × | × | |
氟硅酸, 70 ℉ | × | C | B | C | B | ||||||
乳酸, <50% , 70 ℉ | × | B | A | A | A | × | C | B | B | A | A |
乳酸, >50% , 70 ℉ | × | B | B | B | B | C | C | B | B | A | A |
乳酸, <5% ,沸点 | × | × | C | B | C | × | × | B | B | A | A |
石灰乳, 70 ℉ | B | B | B | B | A | B | B | B | B | B | B |
氯化镁, 70 ℉ | C | C | B | A | B | C | C | A | A | A | A |
氯化镁, <5% ,沸点 | × | C | C | B | C | C | C | A | A | A | A |
氯化镁, >5% ,沸点 | × | C | × | C | × | C | C | B | B | B | B |
氢氧化镁, 70 ℉ | B | A | B | B | A | B | A | B | B | A | |
硫酸镁 | C | C | B | A | B | B | B | C | C | B | B |
马来酸 | C | C | B | B | B | C | C | B | B | A | |
硫醇 | A | × | A | A | A | × | × | ||||
氯化银, <2% , 70 ℉ | × | × | × | × | × | × | C | B | A | A | |
硝酸银, 70 ℉ | C | × | B | B | B | C | C | ||||
甲醇, 70 ℉ | A | A | A | A | A | A | A | A | A | A | A |
萘磺酸, 70 ℉ | × | C | B | B | B | C | C | B | B | ||
环烷酸,沸点 | C | C | B | B | B | C | C | B | B | ||
氯化镍, 70 ℉ | × | × | C | B | C | C | × | A | B | B | |
硫酸镍 | × | C | B | B | B | C | C | B | A | ||
硝酸 | × | × | B | B | B | × | × | B | B | ||
硝基苯, 70 ℉ | A | C | A | A | A | B | B | B | B | A | |
硝基甲烷, 70 ℉ | A | A | A | A | A | A | A | A | A | A | A |
硝基丙烷, 70 ℉ | A | A | A | A | A | A | A | A | A | A | A |
亚硝酸, 70 ℉ | × | × | × | C | × | × | × | ||||
氧化亚氮, 70 ℉ | C | C | C | C | C | × | × | C | |||
油酸 | C | C | B | B | B | C | C | C | C | C | C |
发烟硫酸, 70 ℉ | B | × | B | B | B | × | × | B | B | B | |
草酸 | × | C | C | B | C | C | C | B | B | × | A |
棕榈酸 | B | B | B | A | B | B | B | ||||
光气, 70 ℉ | C | C | B | B | B | C | C | B | B | ||
磷酸, <10% , 70 ℉ | × | C | A | A | A | C | C | A | A | A | A |
磷酸, >10%~70% , 70 ℉ | × | C | A | A | A | C | C | B | C | B | B |
磷酸, <20% , 175 ℉ | × | C | B | B | B | C | C | A | A | C | B |
磷酸, >20% , 175 ℉ <85% | × | C | C | B | C | C | C | B | C | C | C |
磷酸, <10% ,沸点, <85% | × | C | × | C | C | C | C | C | C | C | C |
酞酸, 70 ℉ | C | B | B | A | B | B | B | B | B | A | A |
酞酐, 70 ℉ | B | C | A | A | A | A | A | A | A | ||
苦味酸, 70℉ | × | × | C | B | C | C | × | B | |||
碳酸钾 | B | B | A | A | A | B | B | B | B | A | A |
氯酸钾 | B | C | A | A | A | C | C | B | A | A | |
氯化钾, 70 ℉ | C | C | B | A | B | B | B | B | B | A | A |
氰化钾, 70 ℉ | B | × | B | B | B | C | C | B | B | ||
重铬酸钾 | B | B | A | A | A | B | B | B | A | A | |
赤血盐 | C | B | B | B | B | B | B | B | B | A | A |
亚赤血盐, 70 ℉ | × | B | B | B | B | B | B | B | B | B | |
氢氧化钾, 70 ℉ | C | C | B | A | B | A | A | B | C | B | A |
次氯酸钾 | × | C | C | B | C | × | × | B | A | ||
碘化钾, 70 ℉ | C | B | B | B | B | B | B | B | B | A | A |
锰酸钾 | B | B | B | B | B | C | B | B | |||
磷酸钾 | C | C | B | B | B | B | B | ||||
海水, 70 ℉ | C | B | B | A | B | A | A | A | A | A | A |
硫酸氢钠, 70 ℉ | × | C | C | B | C | C | C | B | B | B | A |
溴化钠, 70 ℉ | B | C | B | B | B | B | B | B | B | ||
碳酸钠 | B | B | B | A | B | B | B | B | B | A | A |
氯化钠, 70 ℉ | C | B | B | B | B | A | A | B | B | A | A |
氰化钠 | B | × | B | B | B | × | × | B | |||
重铬酸钠 | B | × | B | B | B | B | |||||
乙醇钠 | B | A | A | A | A | A | A | ||||
氟化钠 | C | C | B | B | B | B | B | C | C | B | B |
氢氧化钠, 70 ℉ | B | B | B | A | B | A | A | A | A | A | A |
次氯酸钠 | × | × | C | C | C | × | × | B | A | B | |
乳酸钠, 70 ℉ | B | C | C | C | C | C | C | C | |||
氯化锡, <5% , 70 ℉ | × | C | × | C | × | C | C | B | B | A | A |
氯化锡, >5% , 70 ℉ | × | × | × | × | × | × | × | B | C | B | B |
熔融硫磺, 175 ℉ | × | C | B | B | B | C | C | B | A | ||
二氧化硫, 70 ℉ | B | × | A | A | A | C | C | C | A | A | |
硫酸, <2% , 70 ℉ | C | C | B | B | B | C | C | B | C | ||
硫酸, 2%~40% , 70 ℉ | × | C | B | A | B | C | C | A | A | B | A |
× | C | C | B | C | C | C | A | A | × | A | |
硫酸, 40%~90% , 70 ℉ | × | × | × | B | × | × | × | A | A | × | C |
硫酸, 93%~98% , 70 ℉ | B | × | B | B | B | × | × | B | B | × | C |
硫酸, <10% , 175 ℉ | × | C | × | B | × | × | × | A | C | × | B |
硫酸, 10%~60% 及 80% , 175 ℉ | × | × | × | B | × | × | × | B | C | × | C |
硫酸, 60%~80% , 175 ℉ | × | × | × | × | × | × | × | B | C | × | C |
硫酸, <3/4% ,沸点 | × | × | C | B | C | × | × | B | B | × | B |
硫酸, 3/4%~40% ,沸点 | × | × | × | C | × | × | × | B | C | × | B |
硫酸, 40%~65% 及 >85% ,沸点 | × | × | × | × | × | × | × | × | × | × | × |
硫酸, 65%~85% ,沸点 | × | × | × | × | × | × | × | × | × | × | × |
亚硫酸, 70 ℉ | × | C | C | B | C | × | × | B | B | A | B |
四氯化钛, 70 ℉ | C | C | B | C | C | C | |||||
二氯乙烯,沸点 | B | C | B | B | B | B | B | B | B | A | A |
尿素, 70 ℉ | C | C | B | B | B | C | C | C | C | B | B |
醋酸乙烯酯 | B | B | B | B | B | B | |||||
氯乙烯 | B | C | B | B | B | C | C | C | B | A | |
水,沸点 | B | A | A | A | A | A | A | A | A | A | A |
氯化锌 | C | C | B | A | B | B | B | B | A | A | |
氰化锌 | × | B | B | B | B | B | B | B | B | B | B |
硫酸锌 | × | C | A | A | A | C | C | C | C | A |
责任编辑:王元
《中国腐蚀与防护网电子期刊》征订启事
投稿联系:编辑部
电话:010-82387968
邮箱:ecorr_org@163.com
中国腐蚀与防护网官方 QQ群:140808414
相关文章

官方微信
《中国腐蚀与防护网电子期刊》征订启事
- 投稿联系:编辑部
- 电话:010-62313558-806
- 邮箱:fsfhzy666@163.com
- 中国腐蚀与防护网官方QQ群:140808414
点击排行
PPT新闻
铝合金LDH自修复自抗菌膜层构建
点击数:466
碳钢及合金钢应用与区别
点击数:393